HomeWhat We DoMetalsRequest a QuoteExcess InventoryContact Us


brass 268 - coil slitting


268 - yellow brass

ASTM Spec Number
Nominal
Composition
Density

(a)
Module of Elasticity
(b)
Electric
Conductivity (c)
Thermal
Conductivity (d)
Coefficient of
Thermal Expansion
(e)
B36
Cu 66
Zn 34
.306
15
27
67
11.3
(a)Lbs. per cu in. at 68°F (x 27.68 = gms/cu cm at 20°C)
(b) X 106 PSI, tension (Kgf/mm² = KSI x .7031)
(c) % IACS AT 68°F (20°C) as annealed
(d) BTU•ft. @ 68°F ft²•hr•F (20°C)
(e) Inches/inch/°F x 10-5 from 68°F to 572°F (20°C to 300°C)


tensile strength
yield strength*
elongation
rockwell b hardness*
x1000PSI(N/mm²=KSI x 6.895)
x1000PSI(Kgf/mm²=KSI x .7031)
nominal % in 2in.
(=% in 50 mm.)
Nominal .020" gauge
and over
Annealed
(TM00/AM)
1/4 Hard
(TM01/ ¼ HM)
1/2 Hard
(TM02/ ½ HM)
3/4 Hard
(TM03)
Hard
(TM04/HM)
Ex Hard
(TM05/SHM)
Spring
(TM06/XHM)
Ex Spring
(TM08/XHMS)

44-61

49-59

55-65

62-72

68 -78

79-89

86-95

90-99
23

34

44

53

57

67

71

73
52

42

36

25

19

7

5

5 max
75F

52

65

75

80

86

89

90
* Yield Strength - x1000PSI(Nominal .2% offset)(N/mm²=KSI x 6.895)
* Yield Strength - x1000PSI(Nominal .2% offset or range)(Kgf/mm²=KSI x .7031)

* Rockwell F, 30T, 15N, or H where noted
 